Core TDS sheets

Please see our tutorials and FAQ before posting.
fallguy1000
Very Active Poster
Very Active Poster
Posts: 634
Joined: Tue Jan 12, 2010 12:25 am

Re: Core TDS sheets

Post by fallguy1000 » Wed Dec 06, 2017 12:12 am

Evan-using System 3 Silvertip xtra slow. They told me 140F for 2 hours. I figured 155 was the max my tent would ever hit. Maybe I need to ratchet the high number down some?

Fuzz-tds is technical data sheet

I will try to get the tds uploaded
Attachments
Silvertip C&L X-Slow Hardener TDS.pdf
(276.84 KiB) Downloaded 4 times


My boat build is here -------->

viewtopic.php?f=12&t=62495

User avatar
Evan_Gatehouse
Very Active Poster
Very Active Poster
Posts: 2904
Joined: Tue Aug 27, 2002 1:00 am
Location: Vancouver, BC, Canada

Re: Core TDS sheets

Post by Evan_Gatehouse » Wed Dec 06, 2017 1:21 am

Ok - what I know and recommend about post curing:

- slow ramp rates (increasing & decreasing temp rate of change) are good
- fast ramp rates may lead to part distortion
- 155F probably isn't going to hurt anything but I'd stick with S3's recommendation.
- 140F / 2 hrs is a pretty mild post cure. It will improve resin properties but nothing much (10-15% probably)
- do get a few remote reading thermometers inside the oven
- do use a circulating fan that can withstand high heat to ensure even mixing of air and thus even temps in the oven.
designer: FB11/GV series/ HMD18/